Severe flash in PVA '2079851475616104452
ظاهرة المشكلة
Flash of 0.05-0.1mm at the parting line of PVA injection molded products, width >2mm, requiring secondary trimming
تحليل الأسباب
Injection pressure too high >80MPa, melt overflowing from the parting line; clamping force insufficient; mold parting line fitting gap >0.02mm
الحل
1) Reduce injection pressure to 60-70MPa; 2) Increase clamping force or use a larger tonnage '2079851475616104452 machine; 3) Mold fitting gap <0.02mm; 4) Increase melt viscosity to reduce mold penetration tendency
الخلاصة الأساسية
Flash is caused by high-pressure injection and mold gap; reducing pressure and improving mold fitting are key
هل كان هذا مفيدًا؟
0 شخص وجدوا هذا مفيدًا
شكرًا لك على ملاحظاتك!