Injection Molding
2 visualizaciones
Severe flash in PVA '2079851475616104452
Fenómeno del problema
Flash of 0.05-0.1mm at the parting line of PVA injection molded products, width >2mm, requiring secondary trimming
Análisis de la causa
Injection pressure too high >80MPa, melt overflowing from the parting line; clamping force insufficient; mold parting line fitting gap >0.02mm
Solución
1) Reduce injection pressure to 60-70MPa; 2) Increase clamping force or use a larger tonnage '2079851475616104452 machine; 3) Mold fitting gap <0.02mm; 4) Increase melt viscosity to reduce mold penetration tendency
Conclusión clave
Flash is caused by high-pressure injection and mold gap; reducing pressure and improving mold fitting are key
¿Le ha resultado útil?
0 personas encontraron esto útil