Material Drying
7 visualizaciones
PLA Deep Dehumidification 85℃
Fenómeno del problema
After ordinary drying, PLA extrusion still has filament breakage and bubbles, and the moisture content test still exceeds the standard
Análisis de la causa
Deep moisture in PLA requires low dew point and long dehumidification: fine-denier fiber standards require 85±0.5℃, dew point ≤-55℃, and 4 hours of residence, only then can the moisture content be pressed below 30ppm
Solución
①For high-requirement processes use 85℃×4h, dew point ≤-55℃ deep dehumidification; ②Dual molecular sieve rotor redundant configuration; ③Microwave moisture meter real-time feedback; after adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Conclusión clave
Drying for high-requirement PLA processing is system engineering; dew point -55℃ plus 4 hours of residence is the equipment guarantee for ppm-level moisture; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
¿Le ha resultado útil?
0 personas encontraron esto útil
¡Gracias por sus comentarios!