Extrusion & Post 14 visualizaciones

EEA extruded film has gel particles

Fenómeno del problema
Transparent gel particles of 0.1-0.5mm appearing on the EEA extruded film surface
Análisis de la causa
High molecular weight components in EEA not fully melted during extrusion forming local high crystallization zones; extrusion temperature too low or insufficient mixing
Solución
1) Increase extrusion temperature by 5-10°C to ensure full melting; 2) Increase screw mixing section length; 3) Inspect raw material to ensure consistent grade; 4) Replace with a finer 120-mesh screen to intercept unmelted particles
Conclusión clave
Gel particles are caused by insufficient melting; increasing temperature and mixing is the key