Extrusion & Post
14 visualizaciones
EMA Extruded Film Has Gel Particles
Fenómeno del problema
0.1-0.5mm transparent gel particles appear on the surface of EMA extruded film
Análisis de la causa
High-molecular-weight components in EMA are not fully melted during extrusion, forming local high-crystallinity zones; extrusion temperature low or mixing insufficient
Solución
1) Increase extrusion temperature by 5-10°C to ensure full melting; 2) Increase screw mixing section length; 3) Inspect raw material to ensure consistent grade; 4) Replace with a finer 120-mesh screen to intercept unmelted particles
Conclusión clave
Gel particles are caused by insufficient melting; increasing temperature and mixing are key
¿Le ha resultado útil?
0 personas encontraron esto útil
¡Gracias por sus comentarios!