Insufficient EMA transparency
Fenómeno del problema
EMA film haze >20%, below the 5% transparent packaging requirement
Análisis de la causa
EMA methyl methacrylate content too low with crystalline region scattering; extrusion cooling rate too fast
Solución
1) High MMA content EMA with MMA>20% to lower crystallinity; 2) Lower cooling rate; 3) 0.3wt% nucleating agent for uniform crystallization
Conclusión clave
EMA transparency is affected by MMA content and crystallization scattering