Material Drying 8 visualizaciones

Bubbles in EVA injection molded thick walls

Fenómeno del problema
Dense bubbles 0.1-0.5mm appear inside EVA injection molded thick wall products, concentrated at wall thickness center
Análisis de la causa
Holding pressure insufficient <40MPa or holding pressure time short with thick wall center not compacted; raw material contains moisture; injection speed too fast entrapping air; poor mold venting
Solución
1) Increase holding pressure to 60-80MPa; 2) Extend holding pressure time to fully compact thick walls; 3) Fully dry raw material to moisture <0.02%; 4) Add vent grooves or vent pins to mold; 5) Progressively decelerate injection to avoid air entrapment
Conclusión clave
Thick wall bubbles are caused by insufficient holding pressure, moisture and poor venting combined