Extrusion & Post 14 visualizaciones

Die deposit and carbon buildup in EVA extrusion

Fenómeno del problema
After EVA extrusion shutdown, brown carbon deposit layer found on die inner wall; after restarting, black specks on product surface
Análisis de la causa
EVA oxidatively decomposes and carbonizes under prolonged heating in die stagnation zone; die not cleaned in time during shutdown; extrusion temperature too high accelerating carbonization
Solución
1) Flush die with pure PE for 3-5min before shutdown to remove EVA residue; 2) Disassemble and clean die immediately after shutdown; 3) Lower extrusion temperature by 5-10°C to reduce carbonization tendency; 4) Optimize die flow channel to reduce dead zones in stagnation areas
Conclusión clave
Die carbon buildup is caused by thermal oxidation and untimely cleaning; PE flushing and timely cleaning are key