Extrusion & Post 14 visualizaciones

CEF blended with incompatible resin delaminates

Fenómeno del problema
CEF blended with polar resins such as PA/ABS, the extrudate completely delaminates, extremely poor mechanics
Análisis de la causa
CEF and polar resin polarity difference large, compatibility zero, interfacial adhesion extremely low, no compatibilizer used
Solución
1) Use CEF graft compatibilizer CEF-g-MAH 2-5wt%; 2) Add epoxy compatibilizer 1-2wt%; 3) CEF addition amount <10wt%, keep the other resin as continuous phase; 4) Twin-screw high-shear blending to disperse CEF <0.3μm
Conclusión clave
Blends with large polarity differences need reactive compatibilizers to form chemical bonding at the interface to solve
CEF blend delaminationpolarity differenceCEF-g-MAHreactive compatibilizationinterfacial bonding