Extrusion & Post 8 visualizaciones

Dimensional changes of PET injection molded products at high temperature

Fenómeno del problema
PET products show obvious dimensional changes in 80-100°C service environments, causing assembly failure.
Análisis de la causa
Fast cooling during '2079851475616104452 makes crystallization incomplete; post-crystallization at high temperature causes volume shrinkage; annealing is insufficient and mold temperature is on the low side.
Solución
Increase mold temperature to promote full crystallization; fully anneal at 130-140°C/1-2h; select PET grades with high crystallization rate.
Conclusión clave
The high-temperature dimensional stability of PET products depends on sufficient crystallinity.
PETdimensional changepost-crystallizationannealingmold temperature