Extrusion & Post 8 visualizaciones

Stringing and nozzle clogging in PLA 3D printing

Fenómeno del problema
When printing PLA by FDM, the nozzle strings or clogs.
Análisis de la causa
The printing temperature is too high, the melt is too thin and strings, and the retraction is insufficient; or the temperature is too low, the melt is not completely extruded and clogs the nozzle.
Solución
Optimize the printing temperature at 190-210°C; increase the retraction distance to 4-6mm; clean or replace the nozzle.
Conclusión clave
The parameter optimization of PLA 3D printing is the key to printing success.