Fiber content inspection inaccurate

문제 현상
The fiber content measured by the ashing method fluctuates from the formulation value by >3%
원인 분석
PP does not pyrolyze completely during ashing, leaving carbides causing high mass; the glass fiber itself loses mass during high-temperature ashing (>600°C); sampling representativeness is insufficient
해결 방법
Standardize ashing conditions (constant temperature at 550°C for 2 hours); use TGA (thermogravimetric analysis) to accurately measure each component; take samples at multiple points and mix to improve representativeness
핵심 요약
Fiber content is the core indicator of LGFPP quality inspection, and the inspection method needs to be standardized
fiber contentashing methodTGAsampling representativenessquality inspection