Extrusion & Post 8 views

MP extruded pipe ovality exceeding standard

Problem Phenomenon
MP extruded pipe ovality >1.05, exceeding the 1.02 standard requirement
Cause Analysis
pipe cooling uneven, single-side cooling; sizing sleeve design unreasonable; haul-off clamping force uneven causing pipe compression deformation
Solution
1) adopt annular spray cooling to ensure uniform temperature reduction; 2) optimize sizing sleeve inner diameter and taper design; 3) multi-track uniform clamping haul-off; 4) increase vacuum sizing section length to ensure full calibration
Key Takeaway
ovality is caused by uneven cooling and clamping; annular cooling and uniform haul-off are key
MP pipe ovality annular cooling vacuum sizing uniform haul-off