Injection Molding 9 views

Glass fiber exposure of PBT reinforced materials

Problem Phenomenon
The glass fiber on the surface of glass fiber reinforced PBT products is obviously exposed, with a rough feel.
Cause Analysis
The mold temperature is too low, and the surface layer PBT cools quickly and cannot fully coat the glass fiber; the injection speed is too slow; the glass fiber content is too high or the length is too long.
Solution
Raise the mold temperature to 100-120°C; increase the injection speed to achieve fast mold filling; appropriately reduce the glass fiber content or use chopped glass fiber.
Key Takeaway
PBT glass fiber exposure is closely related to mold temperature and mold filling speed.
PBTglass fiber exposuremold temperatureinjection speed