Extrusion & Post
7 visualizações
PCABS FDM printing temperature
Fenómeno do problema
【Problem Phenomenon】PC/ABS filament printing has weak interlayer or deformation, improper parameters
Análise das causas
PC/ABS FDM nozzle 250-270℃, bed temperature 100-110℃, requires an enclosed chamber; higher temperature than pure ABS, interlayer strength depends on full melting
Solução
Nozzle 250-270℃, bed temperature 100-110℃; enclosed chamber; filament dried at 60-80℃ for 4h; after adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Conclusão principal
PC/ABS printing 250-270℃ with an enclosed chamber; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence; include this case in the defect archive as a troubleshooting reference for similar problems later
Isto foi útil?
0 pessoas acharam isto útil
Obrigado pelo seu comentário!