Fenómeno do problema
Internal bubbles of 0.5-2mm in PU elastomer cast products
Análise das causas
Insufficient mixing and degassing; casting temperature too low, viscosity high, bubbles difficult to discharge
Solução
1) Vacuum degassing for 5-10min after mixing; 2) Increase casting temperature to 60-80°C to reduce viscosity and discharge bubbles; 3) Cast slowly to avoid air entrapment
Conclusão principal
PU casting bubbles are caused by insufficient degassing; vacuum degassing is key
PU casting bubbles vacuum degassing casting temperature mixing degassing