Production & Quality
7 visualizações
MP performance degradation after repeated processing
Fenómeno do problema
MP tensile strength decreases 25-30% after 3-4 recycling/reprocessing cycles
Análise das causas
molecular chains break and degrade under repeated high-temperature shear; antioxidants exhausted in multiple processing; cumulative effect of thermo-mechanical degradation
Solução
1) recycled material ratio not exceeding 20-30%; 2) replenish 0.1-0.2wt% antioxidant at each re-extrusion; 3) lower processing temperature 5-10°C; 4) reduce screw speed to reduce shear
Conclusão principal
performance degradation from multiple processing is caused by thermo-mechanical degradation; limiting regrind and replenishing antioxidants are key