Fenómeno do problema
Wavy or snakeskin-like flow marks appear on the surface of PET products.
Análise das causas
Melt temperature is on the low side and the flow front solidifies intermittently; injection speed is slow or unstable; cavity wall temperature is on the low side.
Solução
Increase melt temperature by 10-20°C; appropriately increase injection speed; mold temperature 130-150°C; optimize gate design.
Conclusão principal
PET flow marks are caused by an unstable melt front during filling.
PETflow markmelt frontfillingmold temperature

Isto foi útil?

0 pessoas acharam isto útil

ChemAI