Flash and burrs on products
Fenómeno do problema
Thin sheet-like excess material appears at the mold parting line, affecting assembly
Análise das causas
Clamping force is insufficient to resist cavity pressure; injection pressure peak is too high, causing the mold to open; the mold parting line is worn or has foreign matter
Solução
Verify clamping force ≥ cavity projected area × (40-80MPa); reduce injection/holding peak pressure; check and repair the mold parting line
Conclusão principal
Flash reflects the matching problem between the clamping system and injection pressure
Isto foi útil?