Extrusion & Post
12 Aufrufe
Gel Particles on EVOH Extruded Film
Problembeschreibung
EVOH extruded film surface shows 0.1-0.5mm transparent gel particles
Ursachenanalyse
High molecular weight components in EVOH not fully melted during extrusion forming local highly crystalline regions; extrusion temperature too low or mixing insufficient
Lösung
1) Increase extrusion temperature by 5-10°C to ensure full melting; 2) Increase screw mixing section length; 3) Inspect raw material to ensure consistent grade; 4) Replace with finer 120 mesh screen to intercept unmelted particles
Wichtigste Erkenntnis
Gel particles are caused by insufficient melting; increasing temperature and mixing is key
War das hilfreich?
0 Personen fanden dies hilfreich