Molds & Tooling 8 visualizaciones

PP Sink Mark (Shrinkage)

Fenómeno del problema
Surface depressions behind ribs, bosses, and at thick walls—common on appliance housings.
Análisis de la causa
PP shrinks greatly, and volume shrinkage at thick walls gets no holding pressure compensation; excessive rib thickness ratio, insufficient holding pressure/time, and premature gate freeze-off are direct causes.
Solución
①Control rib thickness to 50%~60% of wall thickness; ②increase holding pressure and extend until gate freeze-off; ③reduce material at thick walls; ④place the gate near thick walls; ⑤strengthen local cooling.
Conclusión clave
PP sink mark = high shrinkage meeting insufficient feeding—treat structure and holding pressure together.
PP;sink mark;shrinkage;holding pressure;rib thickness

¿Le ha resultado útil?

0 personas encontraron esto útil