Extrusion & Post 14 visualizaciones

PVA extruded film has gel particles

Fenómeno del problema
PVA extruded film surface shows 0.1-0.5mm transparent gel particles
Análisis de la causa
High molecular weight components in PVA not fully melted during extrusion form local highly crystalline regions; extrusion temperature on the low side or insufficient mixing
Solución
1) Raise extrusion temperature by 5-10°C to ensure full melting; 2) Increase screw mixing section length; 3) Inspect raw material to ensure consistent grade; 4) Replace with a finer 120 mesh screen to intercept unmelted particles
Conclusión clave
Gel particles are caused by insufficient melting; raising temperature and mixing are the key
PVA filmgel particlemelting temperaturemixing sectionhigh molecular weight component