Extrusion & Post 13 visualizações

EEA Vacuum Section Material Overflow

Fenómeno do problema
Material overflows at the vacuum vent section during EEA extrusion, vent hole blocked
Análise das causas
EEA melt viscosity is low and overflows at the vacuum section; vacuum section temperature is high, viscosity even lower, aggravating overflow; improper vent hole design
Solução
1) Lower the vacuum section temperature by 5-10°C to increase viscosity; 2) Add a baffle above the vent hole to prevent overflow; 3) Increase screw speed to accelerate conveying and reduce residence
Conclusão principal
Overflow is caused by low melt viscosity; lowering temperature and adding a baffle are key
EEA vacuum section overflow melt viscosity temperature reduction vent baffle