Molding Process 5 views

MP compression molding incomplete curing

Problem Phenomenon
MP melamine resin compression molded products curing degree <90%, surface has bubbles and soft spots
Cause Analysis
curing temperature <150°C, low; curing time insufficient <3min; pressure insufficient <10MPa
Solution
1) raise curing temperature to 150-170°C; 2) extend curing time to 5-8min; 3) compression pressure 15-20MPa
Key Takeaway
MP thermoset curing requires the three parameters of temperature, time and pressure to be sufficient
MP compression molding incomplete curing curing temperature curing time compression pressure